What defects are prone to valve castings?

Column:Technical article Time:2024-07-12


1. Stomata

This is a small cavity formed in the metal by the gas that fails to escape during the solidification process, its inner wall is smooth, contains gas, and has a high reflectivity to ultrasonic waves, but because it is basically spherical or elliptic, that is, a point defect, affecting its reflected amplitude. The pores in the ingot are flattened into area-type defects after forging or rolling, which can be detected by ultrasonic detection.

2. Shrinkage and porosity

When the casting or ingot is cooled and solidified, the volume shrinks, and the cavity defect will be formed in the final solidified part because the liquid metal cannot be supplemented. The large and concentrated void is called the shrinkage hole, and the small and dispersed void is called the loose, they are generally located in the center of the final solidified part of the ingot or casting, and the inner wall is rough, surrounded by many impurities and small pores. Due to the law of thermal expansion and cold contraction, shrinkage holes are bound to exist, but with different processing methods and different shapes, sizes and positions, when it is extended to the casting or ingot body becomes a defect. Ingot in the blank forging if the shrinkage hole is not cut clean and into the forging become residual shrinkage hole (shrinkage hole residual, residual shrinkage pipe).

3. Slag inclusion

The slag or refractory material on the furnace body in the melting process is peeled off into the liquid metal, and is sucked into the casting or ingot body during pouring, forming a slag inclusion defect. Slag inclusion is usually not a single existence, often in a dense state or dispersed at different depths, it is similar to volume defects but often have a certain degree of linearity.

4. Inclusion

The reaction products in the smelting process (such as oxides, sulfides, etc.) - non-metallic inclusion, or the addition of some components of the metal composition is not completely melted and remains to form metal inclusion, such as high-density, high-melting point components - tungsten, molybdenum, etc.

5. Segregation

Segregation in castings or ingot mainly refers to the component segregation formed during the smelting process or the melting process of metal because of the uneven distribution of components, the mechanical properties of the area where segregation exists are different from the mechanical properties of the entire metal matrix, and the difference exceeds the allowable standard range to become a defect.

6. Casting cracks

The crack in the casting is mainly caused by the shrinkage stress of the metal cooling and solidification exceeds the ultimate strength of the material, which is related to the shape design of the casting and the casting process, and is also related to the cracking sensitivity caused by the high content of some impurities in the metal material (such as hot brittleness when the sulfur content is high, cold brittleness when the phosphorus content is high, etc.). There will also be an axial intergranular crack in the ingot, and if it cannot be forged in the subsequent open forging, it will remain in the forging and become an internal crack in the forging.

7. Cold insulation

This is a special layered defect in the casting, mainly related to the casting process design, it is in the pouring of liquid metal, due to splashing, turning waves, pouring interruption, or two (or more) strands of metal flow from different directions meet and other reasons, because the liquid metal surface cooling formed by the semi-solid film to remain in the body of the casting and form a diaphragm-like area defect.

8. Turn the skin

This is a layered (area type) defect formed when the liquid metal surface of the first pouring is rapidly cooled in the air to form an oxide film, and the newly poured liquid metal breaks through and turns into the ingot body when continuing to pour, which cannot be eliminated by forging in the subsequent ingot opening forging.

9. Anisotropy

When castings or ingot are cooled and solidified, the cooling speed from the surface to the center is different, so different crystalline structures will be formed, which is manifested as the anisotropy of mechanical properties, and also leads to the anisotropy of acoustic properties, that is, there are different sound speeds and sound attenuation from the center to the surface. The existence of this anisotropy will have an adverse effect on the size and position of defects in ultrasonic inspection of castings.



主站蜘蛛池模板: 国产精品国产a | 欧美一区二区三区中文字幕 | 国产人妻无码一区二区三区不卡 | 欧洲女人牲交视频免费 | 91日韩精品一区二区三区 | 久99久人碰人视频在线 | 日韩a级 | 国产精品久久久久7777婷婷 | 五月婷久久综合狠狠爱97 | 欧美18精品久久久无码午夜福利 | 亚洲高清视频一区二区三区 | 91视视频在线观看入口直接观看 | 天天操天天摸天天爽 | 久久免费99精品国产自在现线 | 国模少妇一区两区三区 | 亚洲aⅴ网站 | 少妇久久久久久被弄到高潮 | 男人操女人免费网站 | 亚洲男同GV在线观看 | 东京热久久综合久久88 | 亚洲国产AV无码专区亚洲AV | 免费无码又爽又高潮视频 | 色播.com| 黄色的视频在线免费观看 | 一级片免费无码 | 国产91欧美| 狠狠躁夜夜躁青青草原软件 | 吃奶呻吟打开双腿做受在线视频 | 国产AV国产精品白丝JK制服 | www.午夜在线b站.com | 2020国产成人综合网 | 第四色成人网 | 日韩av在线第一页 | 91久久国产综合久久91精品网站 | 久久久久91视频 | 欧美极品视频一区二区三区 | 粉嫩一区二区三区国产精品 | 国产精品去看片 | 最近在线更新中文字幕3 | 午夜理论片一级毛片免费 | 亚洲精品专区一区8v |